Project Description

Lead time 20–35 days
Third party SGS / BV / TUV
Quote within 24 hours
Ends plain, bevelled or machined
Anyone can roll a thick wall tube. The reason heavy wall is hard is that the centre of the wall cools more slowly than the surface, and if it cools too slowly it never becomes martensite. The tube then passes a surface hardness check and fails a mid-wall tensile test — which is exactly the failure mode that shows up after the customer has already machined the bore.
So the specification for heavy wall is not “OD × wall × grade”. It is OD × wall × grade × quench route. Below about 25 mm, water quenching with an internal flood usually carries the section. Thinner than that the problem inverts: the section stops being hard to quench and starts being hard to keep round, which is the large diameter thin wall tube case. Between 25 and 50 mm the cooling rate at mid-wall starts to matter and the tempering setpoint has to be adjusted from a section test rather than from a table. Above 50 mm it becomes a project, not a stock item.
This page covers the sizes we hold on a standard route — 219.1 to 355 mm OD, 22 to 50 mm wall — and the larger sizes that are produced to a project schedule. If the tube is going to be bored or honed, say so at enquiry: the machining allowance and the delivered hardness both change, and quoting without that information wastes everyone’s time.
Size matrix
The standard range is what moves on a normal lead time. The project range is produced against mill allocation and is quoted case by case.
Table 1 — OD and wall availability for heavy wall seamless pipe
| OD (mm) | Standard wall (mm) | Project wall (mm) | Status |
|---|---|---|---|
| 219.1 | 22–45 | to 50 | Standard |
| 244.5 | 22–50 | to 60 | Standard |
| 273.0 | 25–50 | to 65 | Standard |
| 298.5 | 28–50 | to 70 | Standard |
| 323.9 | 30–50 | to 80 | Standard |
| 355.6 | 32–50 | to 90 | Standard |
| 406.4 | — | to 100 | Project only |
| 457.0 | — | to 100 | Project only |
| 508.0 | — | to 100 | Project only |
| 610.0 | — | to 100 | Project only |
Project sizes 355–610 mm OD · wall to 100 mm · mill allocation required · project schedule. Wall limits above 355 mm are confirmed per order; they are not stock ranges.
Wall thickness decides whether the core follows the surface
A hardness reading taken at the outside diameter tells you what happened at the surface. It says nothing about the middle of the wall, which is where a heavy section fails first.
Table 2 — Through-thickness risk by wall
| Wall | Quench practice | Core risk | Verification |
|---|---|---|---|
| 22–25 mm | Water, external spray + internal flood | Low | Hardness both ends, tensile per heat |
| 25–35 mm | Water or polymer with agitation | Moderate | Mid-wall hardness on first piece |
| 35–50 mm | Polymer, controlled agitation, longer soak | Core can fall below grade | Section test per heat; tempering adjusted to result |
| 50–100 mm | Project route | High | Destructive section on the trial piece before batch release |
This is why a heavy wall quotation sometimes comes back with a lower maximum wall than the drawing asked for, or with a request to change the grade. It is not a capability limit on the mill — it is a hardenability limit on the section.
Grades that are actually used at this wall
Table 3 — Common grades and their constraint at heavy wall
| Grade | Yield after Q&T | Constraint | Typical use |
|---|---|---|---|
| 27SiMn | ≥835 MPa | Good hardenability; not for welded structures | Cylinder barrel, mining support |
| 42CrMo / 4140 | ≈930–1080 MPa tensile | Needs polymer quench above 35 mm | Heavy mechanical, mould shell |
| 30CrMo | 758–965 MPa (P110 level) | Section test above 30 mm | OCTG body, high load parts |
| P110 | 758–965 MPa | No hardness ceiling, not sour service | High pressure well components |
| Q125 | 862–1034 MPa | Narrow tempering window; project basis at heavy wall | Extreme load, casing |
| E355 / ST52 | 355 MPa min | No hardenability issue; normalised often sufficient | Structural, hydraulic |
Machining allowance: what to leave if the bore will be cut
A heavy wall tube is often bought as cylinder stock, which means the bore will be bored and then honed. The allowance has to cover the decarburised layer, the ovality and the straightness of the as-supplied tube — not just the finish cut.
Table 4 — Typical bore allowance by finished process
| Finished bore process | Radial allowance | Note |
|---|---|---|
| Boring only | 2.5–3 mm | Covers ovality and straightness |
| Boring + honing | 3–5 mm | Honing removes 0.2–0.5 mm after boring |
| Skiving + roller burnishing | 2–4 mm | Needs a stable, fully tempered structure |
| As-supplied bore | — | Scale and decarburisation remain; not a sealing surface |
Ultrasonic acceptance level
Heavy wall is where UT earns its cost, because the defects that matter are internal and the wall is deep enough to hide them. The acceptance level should be stated on the order; “UT according to standard” is not a specification.
Table 5 — UT levels and what they catch
| Level | Reference | Detects | When to specify |
|---|---|---|---|
| L2.5 | GB/T 5777 | Longitudinal and transverse defects, wall thickness | General mechanical, cylinder stock |
| L3 | GB/T 5777 | Tighter acceptance, smaller reflectors | Pressure containment, OCTG body |
| SEP 1921 group 3 | SEP 1921 | Plate and tube equivalent for European orders | German-spec projects |
| Third-party witness | SGS / BV / TUV | Independent verification of the above | When the end user requires it |
Weight per metre, because heavy wall is a lifting problem too
A 610 × 100 tube weighs more than a tonne per metre. That decides the crane, the truck and sometimes whether the tube can be handled at the customer’s site at all.
Table 6 — Approximate mass per metre and per 12 m length
| Size (mm) | kg/m | kg per 12 m | Handling note |
|---|---|---|---|
| 219.1 × 22 | 107 | 1,284 | Standard crane |
| 273.0 × 25 | 153 | 1,834 | Standard crane |
| 323.9 × 32 | 231 | 2,767 | Two-point lift |
| 355.6 × 40 | 311 | 3,734 | Two-point lift |
| 406.4 × 50 | 439 | 5,270 | Heavy lift, spreader required |
| 508.0 × 60 | 663 | 7,954 | Heavy lift, spreader required |
| 610.0 × 100 | 1,258 | 15,092 | Abnormal load; confirm site crane capacity |
Figures use the nominal wall and a density of 7.85 kg/dm³; actual mass varies with wall tolerance.
Where heavy wall is used
Cylinder barrels
Bored and honed after delivery. The delivered hardness has to stay stable through the cut, and the wall has to be thick enough to leave a clean bore.
High pressure and well components
P110 and Q125 sections where the load is carried by the wall and the collapse rating depends on the actual thickness.
Heavy mechanical and mould shells
42CrMo at 35–50 mm wall, machined outside and inside, where a core that did not transform shows up as a soft spot after boring.
Frequently asked questions
What is the thickest wall you can supply?
50 mm on the standard route up to 355 mm OD. Between 355 and 610 mm OD the wall goes to 100 mm on a project basis, with a section test before batch release. Above that it is a dedicated project, not a catalogue item.
Can a 50 mm wall be quenched through?
It can, but not with a generic water quench. Above roughly 25 mm the mid-wall cooling rate falls, so the route uses polymer with controlled agitation and the tempering setpoint is set from a section test rather than from a table.
Can this tube be used directly as cylinder stock?
The bore is not a sealing surface as supplied — it carries scale and a decarburised layer. It is normally bought with a 3–5 mm radial allowance and bored and honed after delivery. Tell us the finished bore and we will set the allowance.
What UT level should I specify?
L2.5 to GB/T 5777 for general mechanical and cylinder stock; L3 for pressure containment and OCTG body. If the order is European, SEP 1921 group 3 is the equivalent language. Third-party witness is available.
Do I need to leave a boring allowance?
If the bore will be machined, yes. The allowance has to cover ovality, straightness and the decarburised layer, not just the finishing cut — typically 2.5–3 mm for boring alone and 3–5 mm for boring plus honing.
How much does one piece weigh?
A 355.6 × 40 × 12 m tube is about 3.7 tonnes; a 610 × 100 × 12 m tube is about 15 tonnes. Confirm the crane capacity at your site before ordering the larger sizes.
What lead time should I plan for?
20–35 days on the standard range. Project sizes depend on mill allocation and the section test, so they are quoted with a schedule rather than a fixed number of days.
What is the minimum order?
One tonne per size on the standard range. Project sizes are usually tied to a full heat, so the minimum is set by the mill allocation rather than by us.
Request a quotation
WhatsApp +86 178 7358 1838
Small OD Thick Wall60–168.3 mm OD, wall 4.5–18 mm, bore Ra ≤1.6 µm.
Engineering MachineryQ460/E355 weldable, 27SiMn for machined parts.
P110 Seamless Tube758–965 MPa, wide band, not for sour service.
C125 Seamless TubeAdded by 5CT Addendum 1, 862–931 MPa.
Q125 Seamless Tube862–1034 MPa, narrow temper window.
Related: alloy steel tube · ASTM A106 pipe