Project Description

Lead time 30–45 days
Third party SGS / BV / TUV
Quote within 24 hours
Certificate EN 10204 3.1 + PMI
Inconel 625 — UNS N06625, W.-Nr. 2.4856 — is a nickel-chromium-molybdenum alloy strengthened by niobium and tantalum rather than by heat treatment. That single design choice explains most of its behaviour: it stays strong from cryogenic temperature to 980 °C, it cannot be hardened or softened by heat treatment after welding, and it tolerates the thermal cycling that would crack a precipitation-hardened alloy. The molybdenum gives it resistance to chlorides and reducing acids, the chromium gives oxidation resistance, and the niobium provides the creep strength that keeps it in jet engine ducting and refinery flare lines. It is also the filler metal of choice for welding 9% nickel steel and duplex stainless, which is why 625 filler sells in a different market from 625 tube.
Chemistry
Table 1 — Chemical composition, ASTM B444 / EN 2.4856 (%, limits)
| Element | Requirement | Function |
|---|---|---|
| Nickel | 58.0 min | Base; austenitic structure and corrosion resistance |
| Chromium | 20.0 – 23.0 | Oxidation resistance and passivity |
| Molybdenum | 8.0 – 10.0 | Chloride pitting and reducing acid resistance |
| Niobium + tantalum | 3.15 – 4.15 | Strengthening and creep resistance; stabilises carbon |
| Iron | 5.0 max | Residual |
| Carbon | 0.10 max | Kept low for weldability and toughness |
| Manganese | 0.50 max | Residual |
| Silicon | 0.50 max | Residual |
| Aluminium | 0.40 max | Residual; also oxide dispersion in powder metallurgy grades |
| Titanium | 0.40 max | Residual |
| Cobalt | 1.0 max | Residual |
| Phosphorus / sulphur | 0.015 / 0.015 max | Restricted for weldability |
Mechanical properties
Table 2 — Room-temperature requirements, annealed
| Property | Requirement | Note |
|---|---|---|
| Yield, 0.2% | 415 MPa min | Annealed condition |
| Tensile | 827 MPa min | — |
| Elongation in 50 mm | 30% min | — |
| Hardness | ≤ 30 HRC typical | Cold worked tube runs higher; state the limit if NACE applies |
| Solution anneal | 1,090 – 1,200 °C, water quench | Required after cold work for corrosion service |
| Creep rupture | To 980 °C | The reason it is used in hot ducting |
Corrosion and high temperature
Table 3 — Service map
| Duty | 625 performance | Comment |
|---|---|---|
| Seawater, including stagnant | Excellent | No pitting or crevice attack at ambient; used for submarine and offshore components |
| Chloride SCC | Immune in practice | Nickel content above 58% puts it outside the austenitic cracking range |
| Oxidation in air | Good to 980 °C continuous | Above that, oxide spalling begins |
| Hydrochloric acid | Moderate | Better than 904L; not for concentrated hot HCl |
| Sulphuric acid | Moderate to good | Depends on concentration and temperature |
| Flue gas and sulphidation | Good | Refinery flare tips and ducting |
| Hydrofluoric acid | Good, with limits | Monel 400 is often better and cheaper for HF |
625 against 825 and 800H
Table 4 — Nickel alloy selection
| 625 (N06625) | 825 (N08825) | 800H (N08810) | |
|---|---|---|---|
| Nickel | 58 min | 38 – 46 | 30 – 35 |
| Chromium | 20 – 23 | 19.5 – 23.5 | 19 – 23 |
| Molybdenum | 8 – 10 | 2.5 – 3.5 | — |
| Strengthening | Nb + Ta in solid solution | Ti-stabilised | Ti-stabilised, coarse grain for creep |
| Yield | 415 MPa | 240 MPa | 180 MPa |
| Best at | Seawater, high temperature, chlorides | Sulphuric and phosphoric acid with chlorides | Creep strength to 1,100 °C |
| Relative cost | Highest | Lower | Lower |
Sizes and forms
Table 5 — Product range
| Form | Range | Standard |
|---|---|---|
| Seamless tube | OD 6 – 219 mm, WT 1 – 20 mm | ASTM B444 / B829 |
| Welded tube | OD 12 – 508 mm, WT 0.8 – 8 mm | ASTM B704 / B705 |
| Pipe | NPS 1/2 – 12, SCH 10 – 160 | ASTM B444 / B705 |
| Length | 3 – 12 m | — |
| Surface | Pickled, bright annealed, or ground | — |
| Fittings | Butt weld fittings in matching grade | B366 |
Welding and fabrication
Table 6 — Welding parameters
| Parameter | Recommendation |
|---|---|
| Filler | ERNiCrMo-3 (matching), or ENiCrMo-3 for SMAW |
| Heat input | Low; 0.5 – 1.5 kJ/mm, stringer beads |
| Interpass | ≤ 150 °C |
| Preheat / PWHT | None; the alloy is not hardenable and PWHT is not applicable |
| Shielding | Argon, or argon + helium; purge the root |
| Post-weld | Pickle and passivate; remove all heat tint before corrosive service |
| Machining | Carbide tooling, low speed, high feed, rigid set-up; work hardening is severe |
Where 625 is the right answer
Seawater piping
Offshore seawater systems, submerged components and heat exchanger tube where copper-nickel and super duplex both fall short.
Flare and vent systems
Flare tips, risers and ducting that see 900 °C plus sulphidation, where 800H lacks the corrosion resistance.
Chemical plant
Reactors and piping in mixed acid service with chlorides, where 904L corrodes.
Nuclear components
Reactor internals and control rod drive mechanisms, where the alloy’s low activation and corrosion resistance are both required.
Bellows and expansion joints
Thin-wall 625 for high-temperature bellows, where fatigue and oxidation act together.
Welding consumables
625 filler for 9% nickel, duplex and dissimilar joints — a different market from tube but the same heat.
Frequently asked questions
Is Inconel 625 the same as Incoloy 825?
No. 625 is N06625 / 2.4856 with 58% nickel and 8–10% molybdenum; 825 is N08825 / 2.4858 with 38–46% nickel, 3% molybdenum and titanium stabilisation. The material numbers differ by one digit and the alloys differ in corrosion performance and price.
Can 625 be heat treated to increase strength?
No. It is strengthened by solid solution and by the niobium-tantalum addition, not by precipitation hardening. Cold work raises strength; annealing at 1,090–1,200 °C restores the soft condition. There is no ageing treatment.
What is the maximum service temperature?
About 980 °C continuous in air for oxidation resistance, and lower when the environment is sulphidising. It retains useful creep strength to that temperature, which is why it is used in exhaust and flare systems where stainless steels creep.
Is 625 suitable for sour service?
Yes, in the annealed condition with hardness controlled, and it is listed in NACE MR0175 / ISO 15156. Cold worked tube may exceed the hardness limit, so state the sour duty and the acceptable hardness at enquiry.
Why is 625 used as a welding filler?
It tolerates dilution from the base metal, keeps toughness at cryogenic temperature, and does not form brittle phases in the weld. That is why it is the standard filler for 9% nickel steel and for dissimilar joints between stainless and carbon steel.
Can 625 be machined?
Yes, but it work-hardens rapidly. Use carbide tooling, low surface speed, high feed and a rigid set-up, and never let the tool rub. A dull tool will harden the surface and ruin the next pass.
What is the difference between 625 tube and 625 filler?
Same alloy family, different product form and different specification. Tube is certified to ASTM B444 or B704 with dimensional and pressure requirements; filler is certified to AWS A5.14 with a chemistry and deposit test. They are not interchangeable paperwork.
What is the minimum order and lead time?
200 kg per size for seamless tube; welded tube from 500 kg. Lead time is 30–45 days depending on size and whether the mill has the heat. PMI and third-party inspection add about a week.
Request a quote
Related products
Incoloy 825 (N08825 / 2.4858)Sulphuric and phosphoric acid with chlorides
Inconel 601 (N06601)Oxidation resistance to 1,200 °C
Hastelloy C276 (N10276)Wet chlorine and mixed acids
904L (N08904 / 1.4539)Super austenitic for acid service
F55 Super DuplexSeawater at lower alloy cost
All nickel alloy tube and pipe · Guide: 625, 825, 400 and C276 — which nickel alloy for which medium
Also in this range: Monel 400 (2.4360) pipe · 904L (1.4539) stainless pipe · F55 (1.4501) super duplex · aerospace stainless tube.
Request a quotation
Give us the form, size, wall, quantity, medium, concentration, temperature and whether NACE applies. State the standard (B444, B704, B705) if the drawing names one.