F55 — S32760 in UNS, 1.4501 in EN — is a 25% chromium super duplex with molybdenum, nitrogen, copper and tungsten, and a pitting resistance equivalent above 40. That number is what puts it into seawater cooling systems, subsea flowlines, riser joints and chemical tanker piping, where 2205 pits and the super austenitic grades do not have the strength. The tungsten and copper are what separate it from 2507: both are 25Cr super duplexes, but F55 is the grade written into NORSOK and many subsea specifications, and its composition is balanced for weld toughness in thick sections. It is a difficult alloy to weld and it cannot be heat treated after welding, so the procedure qualification is part of the product, not an afterthought.
Chemistry
Table 1 — Chemical composition, EN 10088-2 / ASTM A240 (%, limits)
| Element | 1.4501 / S32760 | Function |
|---|---|---|
| Carbon | 0.03 max | Prevents carbide precipitation during welding |
| Chromium | 24.0 – 26.0 | Passive film and pitting resistance |
| Nickel | 6.0 – 8.0 | Balances the ferrite-austenite ratio at about 50/50 |
| Molybdenum | 3.0 – 4.0 | Pitting and crevice corrosion resistance |
| Nitrogen | 0.20 – 0.30 | Strength and pitting resistance; also stabilises austenite |
| Copper | 0.50 – 1.00 | Resistance to reducing acids |
| Tungsten | 0.50 – 1.00 | Additional pitting resistance; the F55 signature |
| Manganese | 1.0 max | Residual |
| Silicon | 0.8 max | Deoxidation |
Mechanical properties
Table 2 — Room-temperature requirements
| Property | Requirement | Note |
|---|---|---|
| Yield, 0.2% | 550 MPa min | Over three times 316L |
| Tensile | 750 MPa min | — |
| Elongation in 50 mm | 25% min | — |
| Hardness | ≤ 32 HRC typical acceptance | Hardness is the practical check on phase balance |
| Impact at −46 °C | 45 J typical | Subsea specifications often require 45 J at −46 °C |
| Ferrite content | 35 – 55% | Measured by metallography; outside this band, toughness or corrosion suffers |
Corrosion performance
Table 3 — Where F55 is specified and where it is not enough
| Duty | F55 performance | Comment |
|---|---|---|
| Seawater, flowing | Good to 60 °C | Standard for seawater cooling and firewater systems |
| Seawater, stagnant or chlorinated | Marginal above 40 °C | Crevice corrosion under deposits is the failure mode |
| Chloride SCC | Resistant to about 100 °C | The reason it replaces 316L in hot chloride service |
| Sour service (H2S) | Listed in NACE MR0175 | Limits depend on partial pressure and temperature |
| Sulphuric acid | Moderate | 904L or 6Mo better in concentrated acid |
| Erosion corrosion | Excellent | Higher hardness and yield than austenitic grades |
F55 against 2507 and 2205
Table 4 — Super duplex grade selection
| 2205 (S32205) | F55 (S32760) | 2507 (S32750) | |
|---|---|---|---|
| Chromium | 22.0 – 23.0 | 24.0 – 26.0 | 24.0 – 26.0 |
| Molybdenum | 3.0 – 3.5 | 3.0 – 4.0 | 3.0 – 5.0 |
| Nitrogen | 0.14 – 0.20 | 0.20 – 0.30 | 0.24 – 0.32 |
| Tungsten | — | 0.50 – 1.00 | — |
| PREN | ≈ 35 | ≥ 40 | ≥ 42 |
| Yield | 450 MPa | 550 MPa | 550 MPa |
| Typical use | Moderate chloride, process plant | Seawater, subsea, sour service | Seawater, higher temperature |
Sizes and forms
Table 5 — Product range
| Form | Range | Tolerance |
|---|---|---|
| Seamless tube | OD 6 – 219 mm, WT 1 – 20 mm | OD ±0.15 mm, WT ±10% |
| Welded tube | OD 12 – 508 mm, WT 0.8 – 10 mm | OD ±0.20 mm |
| Pipe | NPS 1/2 – 24, SCH 10 – 160 | Per A999 / EN 10216-5 |
| Length | 3 – 12 m | +20 / 0 mm |
| Surface | Pickled and passivated | Ra ≤ 1.6 µm |
| Testing | Ferrite count, hardness, corrosion test | ASTM A923 Method A/B/C on request |
Welding: where super duplex fails
Table 6 — Welding parameters
| Parameter | Recommendation |
|---|---|
| Filler | ER2594 (25Cr super duplex) or ER2595 for higher alloy |
| Heat input | 0.5 – 1.5 kJ/mm, narrow band |
| Interpass | ≤ 150 °C, measured not guessed |
| Preheat / PWHT | None; PWHT prohibited |
| Root shielding | Argon with 2–3% nitrogen; nitrogen loss promotes ferrite |
| Post-weld | Pickle and passivate; brush only is not acceptable |
| Qualification | Impact at −46 °C, ferrite count, ASTM A923 corrosion test |
The common failure in F55 fabrication is not the weld metal — it is the heat-affected zone. Too much heat input coarsens the ferrite and drops toughness; too little leaves untempered ferrite and drops corrosion resistance. Both show up in the A923 test, which is why subsea specifications require it rather than accepting a hardness reading alone.
Where F55 is the right answer
Subsea flowlines
Line pipe and jumpers in chlorinated seawater and sour production, where 2205 does not meet the corrosion allowance.
Seawater cooling
Heat exchanger tube and pipework on offshore platforms and FPSOs, the largest single use of the grade.
Firewater systems
Deluge and firewater ring mains where stagnant seawater sits in the line for long periods.
Chemical tankers
Cargo piping and tank heating coils for aggressive chemicals, where the copper addition helps in reducing acids.
Desalination
Brine heater and high-pressure seawater sections, where 2205 pits and 6Mo is not strong enough.
Sour wells
Tubing and surface lines to NACE MR0175, with hardness and ferrite control on every heat.
Frequently asked questions
What is the difference between F55 and 2507?
Both are 25% chromium super duplex with PREN above 40. F55 (S32760 / 1.4501) contains 0.5–1.0% tungsten and 0.5–1.0% copper and is written into NORSOK and many subsea specifications. 2507 (S32750 / 1.4410) has no tungsten, a slightly higher nitrogen range and a PREN of 42 or more. They are not interchangeable without a design review.
Is F55 suitable for seawater?
Yes, in flowing seawater up to about 60 °C, which is why it is the default for offshore cooling and firewater. In stagnant or chlorinated seawater above 40 °C, crevice corrosion under deposits is the limiting mechanism and a higher-alloy grade or a corrosion allowance is needed.
Can F55 be used in sour service?
It is listed in NACE MR0175 / ISO 15156, subject to limits on H2S partial pressure, temperature, pH and chloride content, plus hardness control. State the full sour condition at enquiry — the standard’s acceptance table cannot be applied from the grade name alone.
What ferrite content should the tube have?
35–55%, measured metallographically. Below 35% the corrosion resistance and strength fall; above 55% the toughness and weldability suffer. The mill certificate should state the measured value, not just “balanced”.
Can F55 be heat treated after welding?
No. Solution annealing requires about 1,100 °C and a water quench, which cannot be done on a fabricated spool. PWHT in the 300–900 °C range forms sigma phase and destroys both toughness and corrosion resistance.
What test is required on the weld?
ASTM A923 is the standard: Method A for intermetallic phase, Method B for toughness, Method C for corrosion. Subsea specifications normally require all three plus impact testing at −46 °C and a ferrite count.
Why is F55 more expensive than 2205?
More chromium, molybdenum, nitrogen, tungsten and copper, a narrower process window, and lower mill yield. The premium is roughly 30–50% per tonne, which is usually justified by the corrosion allowance it removes rather than by the strength.
What is the minimum order and lead time?
500 kg per size for seamless tube, 1 tonne for pipe. Lead time is 25–35 days; A923 testing and third-party witness add about a week. Thick-wall and large-diameter sizes run longer.
Request a quote
Related products
2101LDX (S32101 / 1.4162)Lowest nickel lean duplex, 450 MPa
2205 (S32205 / 1.4462)The standard duplex, PREN 35
904L (N08904 / 1.4539)Super austenitic for acid service
254SMO (S31254 / 1.4547)6Mo austenitic for chlorides
Inconel 625 PipeN06625 for the most aggressive seawater
All stainless steel tube · Guide: duplex and super duplex — PREN, phase balance and welding